What happens to a mist eliminator at low flow: turndown, drainage and the traps it sets
11/26/2026A WSA sulphuric acid unit is one of the few places where a mist eliminator sees 98 per cent acid at temperature, in a gas that has just been cooled through the acid dew point. The element at the outlet of the glass-tube condenser is therefore not a generic demister borrowed from a gas plant: its face size, its material and its velocity limit are all set by the acid, not by the gas rate alone. This note covers the square element that fits the standard outlet box, the 2290 by 1930 mm size that appears in most replacement enquiries, and the small mesh rolls used at the tube ends – including the one arrangement that looks right and does not work.
- If you are quoting a drop-in element for the condenser outlet box → What the element actually is
- If someone has copied a clean-gas K value into this duty → Why the velocity limit collapses
- If you have to choose between ETFE and PTFE → ETFE or PTFE
- If the design includes mesh rolls at the glass tube ends → The tube-end mesh roll
Where the mist comes from in a WSA condenser
The process side of a WSA unit is simple to state. Sulphur dioxide in the feed gas is oxidised over a vanadium catalyst to sulphur trioxide, the gas is cooled, and in the condenser the SO3 meets water vapour and becomes sulphuric acid in the vapour phase. That vapour condenses on the inside of vertical glass tubes, runs down as a film, and is collected as 98 per cent acid at the bottom. The gas leaves the tube bundle cool and substantially free of vapour, but not free of liquid.
Two mechanisms put acid into the outlet gas. The first is homogeneous nucleation: as the gas cools through the acid dew point, part of the acid condenses as new submicron particles rather than on the tube wall, typically in the 0.1 to 1 micron range. The second is re-entrainment: the film running down the tubes is sheared at the tube mouths, and where the gas turns out of the bundle, coarse droplets of 10 to 100 microns are thrown off the walls and the tube sheet.
The two fractions need different devices. Coarse droplets are the business of a knitted mesh or a vane pack; submicron mist is the business of fine-fibre media, a candle filter or a wet electrostatic precipitator. A replacement element that is advertised as doing both is either a filter in the shape of a mesh pad, or a mesh pad that will not meet the submicron number. It is worth being explicit about which one is being sold, because the stack test will make the distinction whether the proposal does or not.
What the 2290 by 1930 element actually is
The 2290 by 1930 mm figure is a face size, not a performance figure. It is the clear opening of the outlet box on the condenser, and everything else follows from it: the number of modules the opening is split into, the frame depth, the free area left after framing, and therefore the velocity at a given gas rate.
In round numbers, 2290 by 1930 mm is 4.42 m2 of gross face. A 40 mm frame all round removes about 0.33 m2, leaving 4.09 m2, and the internal mullions of a four-module split take a little more. The practical free area is around 90 per cent of gross, which is the number to use when the gas rate is checked against the velocity limit.
| Item | Typical value | Why it matters |
|---|---|---|
| Gross face | 2290 x 1930 mm, 4.42 m2 | Sets the capacity at a given velocity |
| Free area after framing | about 4.09 m2, 90 per cent | The area the velocity is actually computed on |
| Module split | 4 elements of about 1105 x 925 mm | Handling weight, about 20 kg per module, and replacement without lifting the whole frame |
| Pad thickness | 100 to 150 mm knitted ETFE | Thinner pads drain better in acid; thicker pads buy little extra capture |
| Design velocity | about 1 m/s | Gives roughly 4 m3/s through the element |
| Clean pressure drop | 20 to 30 Pa at 1 m/s | Baseline for the fouling trend |
Two practical consequences follow. First, the element is a box, not a cylinder: the gas distribution across a rectangular face is worse than across a round one, so the corners need attention in the design and the fouling pattern at inspection usually tells you whether the inlet is square to the face or angled. Second, because the element is modular, a replacement can be supplied as four blocks that fit the existing frame, which avoids touching the acid-wetted support structure at all.
Why the velocity limit collapses in acid service
The Souders-Brown expression is the same one used everywhere: maximum velocity equals K times the square root of (liquid density minus gas density) divided by gas density. With 98 per cent acid at about 1840 kg/m3 and condenser outlet gas at about 1.1 kg/m3, the density term is about 40.9. What changes between a clean gas plant and this duty is the K value, and it changes by a factor of three or more.
For clean, low-liquid-load service, knitted mesh is designed around K of 0.107 m/s, giving a maximum of about 4.4 m/s. For acid mist with a heavy liquid load, a fouling tendency and a need to keep the film draining rather than being blown off the mesh, the working K is about 0.03 m/s, giving a maximum near 1.2 m/s and a design velocity near 1.0 m/s. The difference is not conservatism for its own sake: above roughly 1.2 to 1.3 m/s the acid held in the pad stops draining as a film and starts leaving as droplets, which is the failure the element exists to prevent.
This is where copied calculations go wrong. Take the same 4.42 m2 face and apply K of 0.107: the implied capacity is 4.4 m/s, about 19 m3/s through the element. Apply the acid-service K of 0.03 and the honest capacity is about 1 m/s, roughly 4 m3/s. The first number is four to five times the second, and a quotation written on the first number will be a quotation for an element that floods at half its stated duty.
Two checks settle the question for any proposal. Ask which K value was used and why it differs from the clean-gas value; and ask for the velocity at the maximum gas rate, computed on free area rather than gross face. If the answer is above about 1.3 m/s, the element is outside its window before it is installed.
ETFE or PTFE: the temperature line
Both fluoropolymers are effectively inert to 98 per cent sulphuric acid in this temperature range, so the choice is mechanical rather than chemical. ETFE keeps useful strength to about 150 C continuous, is melt-processable, and can be hot-gas welded into frames and seams that hold under load. PTFE goes to about 260 C but cannot be welded; it is sintered or machined, it creeps under sustained load, and a PTFE frame is usually a machined part rather than a welded structure.
The condenser outlet normally runs well below the ETFE limit, so ETFE is the right default: it gives a welded, stiff frame, a lower installed cost and better resistance to the mechanical abuse of installation. PTFE earns its place when the gas temperature can rise – during an upset, a catalyst excursion, or a loss of cooling air – and when the specification has to survive a temperature that nobody can guarantee. A defensible arrangement is an ETFE structure with a stated maximum continuous temperature on the nameplate and an alarm on the outlet temperature, rather than a silent assumption that the outlet will always be cool.
| Material | Continuous limit | 98 per cent acid | Fabrication | Use it when |
|---|---|---|---|---|
| ETFE | about 150 C | good | welded frames, strong | outlet stays below about 120 C |
| PTFE | about 260 C | excellent | sintered, machined, creeps | temperature excursions are possible |
| ECTFE | about 150 C | good | welded, tougher | abrasion or handling damage is a concern |
| Stainless steel | not applicable | attacked when hot | not suitable | never in the acid path |
The tube-end mesh roll and the velocity trap
The glass tube bundle is where the acid is made, and the tube mouths are where it escapes. A film running down a 40 mm bore arrives at the lower end with the gas turning out of the tube and into the outlet plenum. That turn is the moment of maximum shear, and it is the origin of most of the coarse droplets that reach the outlet element.
A short rolled mesh cylinder at each tube end is a reasonable way to break that shear and coalesce the film before it becomes a droplet. It is not a separator, and it will not remove submicron mist; it is a jet breaker with a drainage path. Treated that way, it does useful work at low pressure drop, typically under 15 Pa per roll.
The trap is the placement. A roll pushed into the tube bore sees the full tube velocity. With 40 mm bores and a 4 m3/s gas rate, a bundle of about 1,000 tubes gives roughly 1.26 m2 of bore area and a velocity near 3.2 m/s; a smaller bundle of 500 tubes doubles that to about 6.4 m/s. The acid-service limit for knitted mesh is about 1.2 m/s. A roll inside the bore is therefore operating at three to five times its flooding velocity, and instead of coalescing the film it shreds it into finer droplets – the opposite of the intended effect, and a plausible explanation for a unit that carries more mist after an improvement than before it.
The workable arrangements are the ones where the local velocity is low. Either the roll sits at the tube mouth and protrudes 20 to 30 mm into the plenum, where the jet has expanded and the cross-flow is below the mesh limit, or the element is a larger roll or cartridge in the outlet duct, sized on the duct velocity rather than the tube velocity. Before accepting either, ask for the velocity at the roll, computed on the roll’s own face area, not on the tube area.
Two mechanical details matter as much as the velocity. The roll must be retained against thermal cycling: glass and fluoropolymer expand differently, and a roll that is an interference fit when cold can drop out when hot. And it must not block the acid path: the film has to be able to leave the tube and reach the bottom of the condenser without passing through the mesh, otherwise the roll becomes a dam and the acid backs up into the tube, where it will re-entrain in bursts.
Fit, form and function: what a replacement must reproduce
A replacement element in a licensed unit is judged on three things, and the third is the one that causes trouble. Fit and form are measurable: the face size, the frame depth, the module split, the support grid spacing and the bolting pattern. Function is the pressure drop at the design and maximum gas rates, the velocity at both, the drainage behaviour, and the droplet size the element is claimed to hold.
- Measure the clear opening, not the nominal size. A 2290 by 1930 drawing is often 2285 by 1925 in the field, and a 5 mm interference on a welded fluoropolymer frame is a fit problem that cannot be fixed on site.
- Check the support grid before designing the frame. The element’s weight, plus the acid held in the mesh, has to land on the existing beams; a heavier element on the same grid is a structural change disguised as a like-for-like swap.
- Keep the acid drain path open. The original element has a defined low point and a defined gap to the shell; a replacement that sits 20 mm lower changes the liquid level in the outlet box.
- Match the pressure drop budget, not just the pressure drop. The tail gas train has a fixed draft or blower margin; an element that is 40 Pa cheaper is fine, one that is 200 Pa more expensive is a plant constraint.
- State the removal claim by droplet size. A 99 per cent claim without a size is not a specification; in acid service the number that matters is the cut size, and it should be given at both design and minimum flow.
- Declare the materials in the acid path, including fasteners and gaskets. A single stainless bolt in a hot acid zone is a corrosion source that will be found at the first inspection.
Failure modes that show up in acid service
| Symptom | Usual cause | What to check |
|---|---|---|
| Stack plume or acid deposition after replacement | Element running above its acid-service velocity, or submicron mist no longer removed by the original media | Velocity on free area; what the original element actually was |
| Pressure drop climbing over months | Acid sludge or sulphate scale in the pad, or a partially blocked drain | DP divided by flow squared, plus the drain gap |
| Frame weld cracking | Single-sided welds, no filler, thermal cycling under load | Weld procedure and whether seams are double-welded |
| Mesh rolls found downstream | Interference fit only, no retainer, thermal expansion | Retention method and expansion allowance |
| Carryover at low load only | Gas distribution collapsing upstream, not the element | Velocity profile across the box and the deposit pattern |
What to measure before ordering
Four numbers decide whether a replacement will work, and all four are obtainable without opening the plant: the maximum and minimum gas rate at the outlet box, the gas temperature and density at the same point, the acid load reaching the element in kg per hour, and the clear opening with its support grid. With those, the velocity at both ends of the range, the K value implied, and the pressure drop can all be computed before a drawing is issued.
Two of them are routinely missing from enquiries. Acid load is usually unknown because nobody measures it; a defensible estimate is the acid production rate minus the acid collected, which gives the fraction leaving as mist and film. Minimum gas rate is usually omitted because the unit was sold on a design point; it is the number that decides whether the element will still drain at turndown, and in acid service a pad that stops draining does not fail gently.
Reference
Velocity limits and the K convention used here follow the other notes on this site; the low-flow behaviour of the same element is treated in the note on turndown, and the drainage and seal requirements that decide whether the film reaches the bottom of the vessel are set out in the note on problems that start outside the vessel.
Frequently Asked Questions
Can a knitted mesh element replace a candle filter in a WSA unit?
Not on a like-for-like basis. A candle filter uses fine fibres and works partly by Brownian capture, which is what removes submicron acid mist; a knitted mesh has a much more open structure and holds droplets above roughly 3 to 5 microns. A mesh element can replace a mesh or vane type element, and can take the coarse load upstream of a filter, but it cannot reproduce a submicron guarantee.
Why is ETFE preferred over PTFE here?
Because the outlet gas is normally well below 150 C and the frame has to be welded. ETFE is melt-processable and gives a stiff welded structure; PTFE must be sintered or machined and creeps under load. PTFE is the right choice only when the temperature cannot be guaranteed.
What gas velocity should a 2290 by 1930 element be designed at?
About 1 m/s on free area, which corresponds to a K value near 0.03 m/s for 98 per cent acid at 1840 kg/m3 and gas at 1.1 kg/m3. That is roughly 4 m3/s through the element. Keep the maximum below about 1.3 m/s.
Is a mesh roll inside each glass tube a good idea?
Only if the local velocity is below the mesh limit. Inside a 40 mm bore the velocity is typically 3 to 6 m/s, three to five times the acid-service flooding limit, and the roll will shred the film into finer droplets. Place it at the tube mouth where the jet has expanded, retain it against thermal expansion, and keep the acid drain path clear.
How do I know the element is fouling rather than flooding?
Track pressure drop divided by flow squared. A ratio that rises slowly is fouling; a ratio that stays flat while carryover appears is flooding or a mechanical change. The absolute pressure drop at low load proves nothing, because it falls with the square of flow.
Related notes: the selection map by duty, behaviour at low flow, problems that start outside the vessel, sizing conventions.
- Gas-Liquid Separation Fundamentals — terminology, separation mechanisms and internal selection
- Technical Data Sheet — material and performance reference data
- All Technical Articles — complete engineering index
If you are working on a replacement
A wire mesh pad performs only if it seals to the shell all round, so the measured inside diameter matters as much as the mesh density. See the process data needed to size and select it, what can and cannot be compressed on an urgent replacement and the scope from data review through to delivery.